Feature
It has very good resistance to heat, ENIG, and has excellent insulation, halogen-free. It complies with the Directive 2002/95/EC of the European Parliament and of the Council of 27 January 2003 on the Restriction of the use of certain Hazardous Substances (RoHS) in electrical and electronic equipment.
Product Specification
| LK-ZF600 Serie Components | LK-ZF600 | CA LK-HD600 |
|---|---|---|
| Mixing Ratio | 75 parts | 25 parts |
| Color | Green, Orange-red | White |
| Mixed Properties | ||
| Viscosity | 170 ± 20 dPa.s | |
Processing Parameters
MIXING
LK-ZF600 should be used in a clean environment (20-25°C, 50-60%RH). Use yellow light (UV filtering). Mix 75 parts LK-ZF600 with 25 parts CA LK-HD600. Pot life: 24 hours at ≤ 25°C.
FPC PRE-CLEANING
Pickling → Washing → Sandblasting → Washing → Drying
SCREEN PRINTING
Screen Mesh: 100-130
Screen Mesh Angle: 45°Bias
Mask Thickness: ~20μm (after curing)
Stand-by: 10-30 minutes after printing
Storage & Handling Cautions
(1) Avoid direct sunlight and fire. Store below 15°C for long term. Keep unused film in original packaging (L film: black bag, K film: blue bag).
(2) Avoid contact with: Carbonless copy paper, water, oil, solvents, plasticizers, rubber, or oily handwriting.
(3) Store indicated K films in paper bags; ensure color surfaces do not touch; separate with white paper.
(4) Color samples may fade; scanning images for digital storage is suggested.
(2) Avoid contact with: Carbonless copy paper, water, oil, solvents, plasticizers, rubber, or oily handwriting.
(3) Store indicated K films in paper bags; ensure color surfaces do not touch; separate with white paper.
(4) Color samples may fade; scanning images for digital storage is suggested.
EXPOSURE
Energy:
• For Green: 600mJ/cm² min
• For Orange-red: 500mJ/cm² min
*Exposure depends on substrate and mask thickness. Stand 10-30 mins after exposure.
• For Green: 600mJ/cm² min
• For Orange-red: 500mJ/cm² min
*Exposure depends on substrate and mask thickness. Stand 10-30 mins after exposure.
DEVELOPMENT
• Solution: 1% Sodium Carbonate (pH 10.6 min)
• Temperature: 29 - 31°C
• Spray Pressure: 0.15-0.2MPa
• Dwell Time: 40 - 70 seconds
• Rinsing: 30-50 seconds (water
• Temperature: 29 - 31°C
• Spray Pressure: 0.15-0.2MPa
• Dwell Time: 40 - 70 seconds
• Rinsing: 30-50 seconds (water
FINAL CURE
Temperature: 150°C in conveyorized oven
Time: 60 minutes
Time: 60 minutes
Frequently Asked Questions
What are the primary features of the LK-ZF600 series?
The LK-ZF600 series offers excellent heat resistance, high insulation properties, and is halogen-free. It is fully RoHS compliant and compatible with ENIG processes.
What is the correct mixing ratio for this solder mask?
The mixing ratio by weight is 75 parts of LK-ZF600 to 25 parts of CA LK-HD600. It must be stirred thoroughly before use.
How long can I use the mixture after it has been stirred?
The pot life after mixing is 24 hours, provided it is stored in a dark place at a temperature of ≤ 25°C (77°F).
What exposure energy is recommended for different colors?
For the Green variant, a minimum of 600mJ/cm² is required. For the Orange-red variant, a minimum of 500mJ/cm² is recommended under the phototool.
What are the critical environmental conditions for processing?
Processing should occur in a clean room at 20-25°C with 50-60%RH. Lighting must be yellow (UV filtered) to prevent premature curing.
What is the final curing requirement?
The final cure requires 60 minutes at a temperature of 150°C in a conveyorized oven to ensure full mechanical and chemical properties.